I spent two hours this evening turning an almost 100kg bucket of wheelweights into over 60kg of ingots and decided to take some pics. This is not intended to be a primer on smelting, just shows what I think is a pretty typical and effective setup.
Pic 1 - Wheelbarrow to throw hot waste into, Camp Burner from Lebaron, Stock Pot, Propane Tank
Pic 2 - What you get from the Garage or Tire Store. Mostly Wheelweights, but also paper, rubber, dirt, and the odd Zinc Wheelweight (these are bad - more later). If there is any moisture or oil (i.e. liquids), they must be eliminated before the smelting occurs
Pic 3 - some of the stuff you need to remove beforehand
Pic 4 - Lead is very dense, so all the junk will conveniently float on top, ready to be scooped off with a Ladle Sieve
Pic 5 - a Zinc Wheelweight. These are bad for bullet alloy and must be culled. I used to try to pick them out by hand, but as l was only finding three or four per 100kg, and they are not all as easy to identify as the one in the pic, I found a better way. Zinc has both a higher melting point than Lead (420 deg C vs. 328 deg C), and is only about 2/3 as dense, so if you are careful and keep the temp to about 350-400 deg C, the zinc wheelweights just skim off like this one did.
Pic 6 - Lead with junk skimmed off
Pic 7 - my Dollar Store Utensils. The Ladle Sieve is used to remove the stuff floating on top, and the Soup Ladle is used to pour the molten Lead into my Ingot Mold. A full Ladle weighs about 1 1/2 kg, and first time I scooped lead with it, I couldn't believe how heavy it felt (Lead is 11 1/2 times as dense as water).
Pic 8 - My Ingot Mold. An Aluminum Muffin tin (thanks again Dollar Store). The Aluminum is soft when hot, so it takes some care when handling. I have since changed to steel - much better.
Pic 9 - The finished product. The Ingots are about 4 lbs, 2lbs and 1 lb in weight - good sizes for handling and use.
Pic 1 - Wheelbarrow to throw hot waste into, Camp Burner from Lebaron, Stock Pot, Propane Tank
Pic 2 - What you get from the Garage or Tire Store. Mostly Wheelweights, but also paper, rubber, dirt, and the odd Zinc Wheelweight (these are bad - more later). If there is any moisture or oil (i.e. liquids), they must be eliminated before the smelting occurs
Pic 3 - some of the stuff you need to remove beforehand
Pic 4 - Lead is very dense, so all the junk will conveniently float on top, ready to be scooped off with a Ladle Sieve
Pic 5 - a Zinc Wheelweight. These are bad for bullet alloy and must be culled. I used to try to pick them out by hand, but as l was only finding three or four per 100kg, and they are not all as easy to identify as the one in the pic, I found a better way. Zinc has both a higher melting point than Lead (420 deg C vs. 328 deg C), and is only about 2/3 as dense, so if you are careful and keep the temp to about 350-400 deg C, the zinc wheelweights just skim off like this one did.
Pic 6 - Lead with junk skimmed off
Pic 7 - my Dollar Store Utensils. The Ladle Sieve is used to remove the stuff floating on top, and the Soup Ladle is used to pour the molten Lead into my Ingot Mold. A full Ladle weighs about 1 1/2 kg, and first time I scooped lead with it, I couldn't believe how heavy it felt (Lead is 11 1/2 times as dense as water).
Pic 8 - My Ingot Mold. An Aluminum Muffin tin (thanks again Dollar Store). The Aluminum is soft when hot, so it takes some care when handling. I have since changed to steel - much better.
Pic 9 - The finished product. The Ingots are about 4 lbs, 2lbs and 1 lb in weight - good sizes for handling and use.
Last edited: